Investasi Casting Foundry | Pengecoran Pasir saka China

Casting Stainless Steel, Casting Wesi Gray, Casting Besi Ulet

Perawatan Panas saka Casting Baja Karbon

Cara perawatan panas biasane digunakake kanggo casting baja karbon yaiku: annealing, normalizing utawa normalizing + tempering. Pengaruh saka telung cara perawatan panas iki ing sifat mekanik baja karbon cast ditampilake ing gambar ing ngisor iki.

Kekuwatan Tensile Casting Baja Karbon sawise Perawatan Panas

Suhu Annealing lan Kekerasan Casting Baja Karbon
Kelas Baja Karbon Kandungan Karbon /% Suhu Annealing / ℃ Tahan Wektu Metode Cooling Kekerasan / HBW
Ketebalan dinding / mm Wektu / h
ZG200 - 400 0.10 - 0.20 910 - 880 < 30 1 Cooling kanggo 620 ℃ ing furnaces banjur cooling ing udhara 115 - 143
ZG230 - 450 0.20 - 0.30 900 - 870 133 - 156
ZG270 - 500 0.30 - 0.40 890 - 860 143 - 187
ZG310 - 570 0.40 - 0.50 870 - 840 30 - 100 nambah 1 jam / 30 mm 156 - 127
ZG340 - 640 0,50 - 0,60 860 - 830 187 - 230

 

Sifat mekanik baja tuang sing dinormalisasi rada luwih dhuwur tinimbang baja tuang anil. Amarga tingkat undercooling sajrone transformasi struktur kasebut relatif gedhe, kekerasan bakal luwih dhuwur, lan kinerja pemotongan uga luwih apik.

Kekuwatan Ngasilake Casting Baja Karbon sawise Perawatan Panas

Normalisasi lan Kekerasan Casting Baja Karbon
Kelas Baja Karbon Kandungan Karbon (%) Normalisasi Suhu / ℃ Tempering Kekerasan / HBW
Suhu / ℃ Metode Cooling
ZG200 - 400 0.10 - 0.20 930 - 890 540 - 610 ing tungku utawa hawa 126 - 149
ZG230 - 450 0.20 - 0.30 930 - 890 540 - 610 ing tungku utawa hawa 139 - 169
ZG270 - 500 0.30 - 0.40 890 - 860 550 - 620 ing tungku utawa hawa 149 - 187
ZG310 - 570 0.40 - 0.50 890 - 850 550 - 650 ing tungku utawa hawa 163 - 217
ZG340 - 640 0,50 - 0,60 870 - 830 550 - 650 ing tungku utawa hawa 187 - 228

 

Kanggo casting baja karbon karo isi karbon dhuwur lan wangun Komplek, kanggo ngilangke kaku ampas lan nambah kateguhan, perawatan tempering bisa digawa metu sawise normalizing. Suhu tempering umume 550 ℃ -650 ℃, banjur adhem ing udhara.

Elongation saka Casting Carbon Steel sawise Perawatan Panas

Nalika isi karbon luwih saka 0,35%, bagean baja karbon cast uga bisa quenched lan tempered (quenched + suhu dhuwur tempered). Castings baja karbon cilik bisa langsung quenched lan tempered ing negara minangka-cast; casting baja karbon gedhe utawa Komplek-shaped kudu quenched lan tempered sawise normalizing.

Bagean Shrinkage saka Carbon Steel Castings sawise Perawatan panas

 

Suhu Quenching lan Tempering lan Kekerasan Casting Baja Karbon
Kandungan karbon% Suhu Quenching / ℃ Suhu Tempering / ℃ Kekerasan Sawise Tempering / HBW
0.35 - 0.45 (Batch Cilik) 850 - 830 (Pendingin ing Banyu) 300 - 400 364 - 444
400 - 450 321 - 415
510 - 550 241 - 286
540 - 580 228 - 269
580 - 640 192 - 228
0.45 - 0.55 (Batch Cilik) 830 - 810 (Pendingin ing Banyu utawa Lenga) 550 - 630 220 - 240
450 ≈ 269
550 ≈ 248
650 ≈ 228
0.30 - 0.40 (Batch Massa) 840 -880 (Pendingin ing Banyu utawa Lenga) 520 - 550 229 - 269
530 - 560 217 - 255
540 - 570 207 - 241
550 - 580 187 - 229
0.40 - 0.50 (Batch Massa) 820 - 840 (Pendingin ing Banyu utawa Lenga) 530 - 560 229 - 269
550 - 580 217 - 255
560 - 590 207 - 241
570 - 600 187 - 229

 

 


Wektu kirim: Jul-23-2021
.